Close-up of a fired ceramic bowl showing glaze crawling — bare clay patches where the glaze has pulled back, earthy tones, soft natural light on a wooden studio surface

What crawling actually is

Crawling is delamination during the melt. The glaze coating fractures or rolls up on itself before it has time to flow back and heal, leaving bare patches of clay body exposed on the fired surface. It is not random. Every crawl has a cause you can trace, and once you trace it, you can fix it.

The mechanism is straightforward: the molten glaze has a surface tension that pulls it toward itself. If adhesion between the melt and the clay body is too weak — or if the dried raw glaze layer cracks before the kiln reaches melting temperature — surface tension wins and the glaze beads away from the break.

The five main causes

### 1. Dusty, oily, or contaminated bisque

This is the most common cause and the easiest to overlook. Any layer of kiln dust, skin oil, mould-release, wax overspray, or even fingerprints reduces the mechanical bond between the raw glaze and the bisqueware.

Diagnosis: Crawling concentrated at finger-contact areas, rim edges that were handled, or the lower half of a pot that sat in dusty storage.

Fix: - Wipe bisqueware with a clean damp sponge before glazing. Let it dry fully. - For heavy contamination, wash pieces and allow 24 h of drying at room temperature. - Keep bisque stored rim-down or covered in a dust-free area. - Wax resist applied too close to a glazed surface is a frequent offender — maintain a sharp, clean boundary.

### 2. Glaze applied too thick

A thick raw glaze coat shrinks more during drying and especially during the early stages of firing (400–600 °C) when organic binders burn out. High shrinkage generates tensile stress in the layer. If that stress exceeds the coating's green strength, it cracks — and those cracks become crawl lines once the glaze melts.

Diagnosis: Visible cracking or lifting of the raw glaze before the kiln is even loaded. Run a fingernail lightly across the dried surface — if flakes lift easily, it's too thick. Measure specific gravity: most brushing glazes run 1.40–1.50 g/mL; dipping glazes 1.35–1.45 g/mL. Above those ranges, dilute.

Fix: - Adjust slop consistency and check specific gravity with a hydrometer every session. - Apply in two thin coats rather than one heavy coat, allowing each to dry completely. - For high-alumina or heavily opacified glazes (which are naturally prone to this), consider adding a small amount of CMC gum (0.1–0.2 % by weight on dry batch) to improve green strength.

### 3. Excess plastic materials in the recipe

Plastic clays — ball clay, kaolin, bentonite — are essential for glaze suspension but they carry a cost: high raw shrinkage. Ball clay shrinks roughly 6–7 % on drying; bentonite can exceed 10 %. In a glaze recipe, every percent of bentonite above about 2 % raises crawl risk significantly.

In UMF terms, the alumina source matters. If you're pulling Al₂O₃ primarily from plastic kaolin rather than calcined kaolin or feldspar, you are loading shrinkage into the recipe unnecessarily.

Diagnosis: A glaze that crawls consistently regardless of application thickness or bisque prep, especially one with high clay additions for suspension.

Fix: - Replace part of the raw kaolin with calcined kaolin (same Al₂O₃ and SiO₂ contribution, near-zero shrinkage). A 50/50 split of raw to calcined kaolin is a standard starting point. - Cap bentonite at 1.5–2.0 % and use a gum (CMC or Veegum T) to compensate for lost suspension. - Check the recipe's total plastic clay content. If it exceeds 20–25 % of the batch, substitution is warranted.

### 4. Surface tension of the melt

Surface tension in a silicate melt is governed primarily by the flux system. Glazes high in CaO have relatively high surface tension. Glazes with significant B₂O₃, Li₂CO₃, or ZnO tend toward lower surface tension and better wetting of the clay body.

This does not mean you should eliminate calcium — it is a critical flux for durability and hardness. But if a recipe is already prone to crawling, examine the flux balance.

OxideEffect on surface tension
CaOIncreases
MgOIncreases (moderate)
B₂O₃Decreases
Li₂ODecreases
ZnODecreases (moderate)
K₂O / Na₂OModerate, varies with temp

The Stull chart plots Al₂O₃ vs SiO₂ in UMF and correlates with melt fluidity. A glaze sitting in the low-silica, low-alumina region will have a runny, low-viscosity melt that may heal crawl cracks; one in the high-alumina region will be stiffer and less forgiving. See the Stull chart explained for how to read your recipe's position.

### 5. Firing rate through the critical range

Firing too fast through 200–600 °C traps steam and volatilizes binders violently, blowing micro-craters in the raw layer before it sinters. Even a glaze with reasonable shrinkage can crawl if it arrives at the melt stage already fractured.

Fix: - Use a slow climb segment: 55–80 °C/h from room temperature to 600 °C, or program a one-hour hold at 120 °C to drive off residual moisture. - This is especially important for thick-walled work and freshly dipped ware that wasn't fully dry before loading.

A base recipe prone to crawling — and its fix

Here is a cone 6 oxidation satin matte that illustrates the problem. The original version used 25 % ball clay for suspension and crawled reliably on flat tiles.

Problematic original (crawls):

Material%
Custer feldspar40
Silica (325 mesh)15
Whiting15
Ball clay25
Zinc oxide5
Total100

Revised version (reduced crawl risk):

Material%
Custer feldspar40
Silica (325 mesh)15
Whiting15
Ball clay10
Calcined kaolin15
Zinc oxide5
Total100

Add colorants on top of the 100 % base. The substitution keeps the Al₂O₃ and SiO₂ contribution nearly identical while cutting raw shrinkage by roughly half. Add 0.15 % CMC gum (dry weight) if suspension becomes an issue.

This is a starting point. Run a triaxial blend with varying calcined/raw kaolin ratios (e.g. 0/25, 10/15, 15/10, 20/5, 25/0) on your actual clay body before committing to production. What crawls on a porcelain may be fine on a stoneware with a rougher bisque surface.

Diagnosis checklist

  • Where is the crawl? Rims and handles = contamination or handling. Broad flat areas = thickness or shrinkage. Consistent pattern = recipe.
  • When did you see it? Raw glaze cracking in the bucket = too thick or too much plastic. No sign until after firing = surface tension or fast firing.
  • Has anything changed? New batch of ball clay (different particle size = different shrinkage). New bisque temperature. Different water source (hardness affects gum performance).
  • Is it only on certain forms? Horizontal surfaces hold more glaze by gravity during dipping and are thicker. Concave interiors trap air during pouring.

Food safety note

Bare clay patches exposed by crawling are not simply an aesthetic defect. The raw, unglazed clay is porous and cannot be rendered food-safe by any post-firing treatment. Pieces intended for food use must be refired with the crawl filled — apply a small amount of glaze to the bare patch, dry completely, and refire. Per ASTM C738 (lead extraction) and ASTM C927 (cadmium extraction) standards for ceramic tableware, the entire food-contact surface must carry a continuous, properly melted glaze coating to be evaluated for release compliance. If the crawl is on a non-food-contact exterior surface only, it is a cosmetic issue; still, assess whether the exposed clay will absorb moisture in service.

Quick-reference fixes

  • Dusty bisque → clean with damp sponge, dry fully before glazing
  • Too thick → adjust specific gravity, two thin coats, add CMC
  • Excess plastic → swap half the raw kaolin for calcined kaolin, cap bentonite at 2 %
  • High surface tension melt → review flux balance, consider partial B₂O₃ or Li₂O substitution
  • Fast firing → slow segment to 600 °C, hold at 120 °C for moisture
  • Contamination → audit wax, mould release, storage conditions

For the broader picture of how oxide ratios affect melt behavior, glaze chemistry 101: understanding UMF is worth reading before you adjust a flux.

---

Ready to build a crawl-resistant recipe from scratch? Upload a glaze photo or start a new recipe on kilnmuse →

Ready to put this into practice?

Generate an original glaze recipe from a photo. Automatic chemistry validation plus variants to bench-test.

Generate a recipe free →